{"id":2729,"date":"2026-07-17T02:22:54","date_gmt":"2026-07-17T02:22:54","guid":{"rendered":"https:\/\/zhiweichem.com\/?p=2729"},"modified":"2026-07-17T02:22:57","modified_gmt":"2026-07-17T02:22:57","slug":"cellulose-ether-in-cementitious-grout","status":"publish","type":"post","link":"https:\/\/zhiweichem.com\/pt\/cementitious-grout\/cellulose-ether-in-cementitious-grout\/","title":{"rendered":"Qual \u00e9 o papel do \u00e9ter de celulose na argamassa ciment\u00edcia?"},"content":{"rendered":"<figure class=\"wp-block-image aligncenter size-large\"><img fetchpriority=\"high\" decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"Aplica\u00e7\u00e3o de \u00e9ter de celulose em argamassa ciment\u00edcia\" class=\"wp-image-2733 lazyload\"\/><noscript><img decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-1024x576.webp\" alt=\"Aplica\u00e7\u00e3o de \u00e9ter de celulose em argamassa ciment\u00edcia\" class=\"wp-image-2733\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-1536x865.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Application-at-a-Construction-Site.webp 1890w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose ajuda<a href=\"https:\/\/zhiweichem.com\/pt\/conhecimento\/low-temperature-early-strength-cementitious-grout-formula\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/knowledge\/low-temperature-early-strength-cementitious-grout-formula\/\" rel=\"noreferrer noopener\"> argamassa ciment\u00edcia<\/a> ret\u00eam \u00e1gua, resistem \u00e0 hemorragia, mant\u00eam a coes\u00e3o e permanecem male\u00e1veis durante a aplica\u00e7\u00e3o. No entanto, o \u00e9ter de celulose n\u00e3o melhora todas as propriedades em todas as dosagens.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um tipo de argamassa com viscosidade muito baixa pode n\u00e3o proporcionar espessamento suficiente para impedir a segrega\u00e7\u00e3o. Um tipo de argamassa com viscosidade muito elevada pode reduzir tanto o fluxo que a argamassa n\u00e3o consegue preencher espa\u00e7os estreitos. Uma dosagem excessiva tamb\u00e9m pode introduzir mais ar, aumentar a porosidade e reduzir a resist\u00eancia inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O objetivo principal n\u00e3o \u00e9, portanto, utilizar a viscosidade mais elevada nem a quantidade maior. O objetivo \u00e9 encontrar um equil\u00edbrio entre fluidez, estabilidade, reten\u00e7\u00e3o de \u00e1gua e resist\u00eancia.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Este equil\u00edbrio \u00e9 especialmente importante em argamassas sem retra\u00e7\u00e3o, argamassas para funda\u00e7\u00f5es de equipamentos, argamassas de fixa\u00e7\u00e3o, argamassas para liga\u00e7\u00e3o de pr\u00e9-fabricados e outros sistemas ciment\u00edcios que requerem tanto uma elevada fluidez como uma estrutura endurecida uniforme.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O que \u00e9 a argamassa ciment\u00edcia?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A argamassa ciment\u00edcia \u00e9 uma<a href=\"https:\/\/zhiweichem.com\/pt\/hemc\/fornecedor-de-hemc-para-argamassa-de-mistura-seca\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/hemc\/hemc-for-dry-mix-mortar-supplier\/\" rel=\"noreferrer noopener\"> material de mistura a seco<\/a> que se transforma numa pasta fluida ou de consist\u00eancia fluida ap\u00f3s a adi\u00e7\u00e3o de \u00e1gua. Normalmente cont\u00e9m cimento, agregados classificados, enchimentos minerais, componentes de expans\u00e3o, agentes redutores de \u00e1gua, aditivos de controlo da presa e pequenas quantidades de pol\u00edmeros funcionais.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os empreiteiros utilizam argamassa ciment\u00edcia para preencher fendas e transferir cargas. As aplica\u00e7\u00f5es mais comuns incluem:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Inje\u00e7\u00e3o de cimento por baixo das placas de base das m\u00e1quinas<\/li>\n\n\n\n<li>Preenchimento de espa\u00e7os vazios sob colunas de a\u00e7o<\/li>\n\n\n\n<li>Fixa\u00e7\u00e3o de parafusos de ancoragem<\/li>\n\n\n\n<li>Liga\u00e7\u00e3o de componentes pr\u00e9-fabricados de bet\u00e3o<\/li>\n\n\n\n<li>Repara\u00e7\u00e3o de cavidades no bet\u00e3o<\/li>\n\n\n\n<li>Preenchimento de espa\u00e7os estreitos em torno de elementos estruturais<\/li>\n\n\n\n<li>Apoio a apoios de pontes e equipamento industrial<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">A argamassa fresca deve fluir para estes espa\u00e7os sem vibra\u00e7\u00e3o excessiva. Deve tamb\u00e9m manter-se uniforme enquanto flui. Se a \u00e1gua subir \u00e0 superf\u00edcie ou se part\u00edculas pesadas se depositarem, a argamassa pode apresentar zonas fracas, canais de retra\u00e7\u00e3o e resist\u00eancia irregular.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/zhiweichem.com\/pt\/empresa\/hpmc-vs-hemc\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/company\/hpmc-vs-hemc\/\" rel=\"noreferrer noopener\">\u00c9ter de celulose<\/a> ajuda a controlar estes problemas relacionados com o estado de frescura.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Por que raz\u00e3o a argamassa ciment\u00edcia necessita de \u00e9ter de celulose?<\/h2>\n\n\n\n<figure class=\"wp-block-image aligncenter size-large\"><img decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"Mat\u00e9rias-primas e \u00e9ter de celulose para argamassa ciment\u00edcia\" class=\"wp-image-2737 lazyload\"\/><noscript><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-1024x576.webp\" alt=\"Mat\u00e9rias-primas e \u00e9ter de celulose para argamassa ciment\u00edcia\" class=\"wp-image-2737\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-1536x864.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Raw-Materials-Used-in-Cementitious-Grout.webp 1891w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Uma argamassa de alto fluxo cont\u00e9m \u00e1gua e superplastificante em quantidade suficiente para se deslocar atrav\u00e9s de um espa\u00e7o restrito. Esta condi\u00e7\u00e3o de fluidez cria um risco de sangramento e segrega\u00e7\u00e3o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A \u00e1gua pode subir, enquanto o cimento e a areia descem. A mistura pode parecer fluida \u00e0 primeira vista, mas a sua estrutura interna \u00e9 inst\u00e1vel. Ap\u00f3s o endurecimento, as sec\u00e7\u00f5es superior e inferior podem apresentar densidades e propriedades mec\u00e2nicas diferentes.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose aumenta a viscosidade da fase aquosa. Al\u00e9m disso, melhora a capacidade da pasta de manter as part\u00edculas de cimento, os enchimentos e os agregados finos numa suspens\u00e3o uniforme.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um \u00e9ter de celulose adequado pode proporcionar cinco vantagens importantes.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">1. Melhor <a href=\"https:\/\/zhiweichem.com\/pt\/mortar\/how-does-hydroxypropyl-methylcellulose-affect-mortar\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/mortar\/how-does-hydroxypropyl-methylcellulose-affect-mortar\/\" rel=\"noreferrer noopener\">Reten\u00e7\u00e3o de \u00e1gua<\/a><\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O cimento necessita de \u00e1gua para a hidrata\u00e7\u00e3o. Se o substrato, o agregado seco, o vento ou uma temperatura elevada retirarem a \u00e1gua demasiado rapidamente, a hidrata\u00e7\u00e3o fica incompleta.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose ret\u00e9m parte da \u00e1gua de mistura no interior da argamassa. Esta a\u00e7\u00e3o ajuda a manter um n\u00edvel de humidade mais est\u00e1vel durante a aplica\u00e7\u00e3o e a cura inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Uma melhor reten\u00e7\u00e3o de \u00e1gua pode contribuir para:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Hidrata\u00e7\u00e3o mais uniforme do cimento<\/li>\n\n\n\n<li>Melhor contacto com o substrato<\/li>\n\n\n\n<li>Menor risco de secagem r\u00e1pida da superf\u00edcie<\/li>\n\n\n\n<li>Maior consist\u00eancia durante o per\u00edodo de trabalho<\/li>\n\n\n\n<li>Desempenho mais est\u00e1vel em espa\u00e7os estreitos e em \u00e1reas absorventes<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">No entanto, uma reten\u00e7\u00e3o de \u00e1gua muito elevada nem sempre \u00e9 melhor. Uma dosagem elevada pode atrasar a liberta\u00e7\u00e3o de \u00e1gua, alterar o comportamento de presa ou aumentar o teor de ar da mistura. O formulador deve confirmar o resultado final atrav\u00e9s de ensaios laboratoriais.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">2. Redu\u00e7\u00e3o do sangramento e da segrega\u00e7\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A separa\u00e7\u00e3o por sangramento ocorre quando a \u00e1gua se separa dos materiais s\u00f3lidos e sobe para a superf\u00edcie. A segrega\u00e7\u00e3o ocorre quando os componentes s\u00f3lidos deixam de se manter distribu\u00eddos uniformemente.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Uma argamassa ciment\u00edcia sem um controlo adequado da viscosidade pode apresentar ambos os problemas. O material fresco pode sofrer separa\u00e7\u00e3o durante a mistura, o transporte ou a aplica\u00e7\u00e3o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose forma uma rede interna fraca na fase aquosa. Esta rede ajuda a manter o cimento e o agregado fino em suspens\u00e3o. Pode reduzir a separa\u00e7\u00e3o vis\u00edvel da \u00e1gua e produzir uma sec\u00e7\u00e3o transversal endurecida mais uniforme.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A melhoria depende da viscosidade e da dosagem. Um tipo de produto de baixa viscosidade, quando utilizado numa dosagem muito baixa, pode n\u00e3o criar estrutura suficiente. Um tipo de produto de alta viscosidade pode impedir o sangramento, mas tamb\u00e9m pode reduzir o fluxo necess\u00e1rio.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">3. Maior coes\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Uma argamassa est\u00e1vel deve mover-se como um material cont\u00ednuo. N\u00e3o deve libertar \u00e1gua \u00e0 volta da borda da \u00e1rea de espalhamento. Tamb\u00e9m n\u00e3o deve deixar part\u00edculas grossas para tr\u00e1s \u00e0 medida que a pasta avan\u00e7a.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose aumenta a coes\u00e3o entre as fases l\u00edquida e s\u00f3lida. Este efeito pode conferir \u00e0 argamassa um aspeto mais liso e uniforme durante a mistura e o vertimento.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Uma boa coes\u00e3o \u00e9 particularmente importante quando a argamassa tem de percorrer um espa\u00e7o longo ou estreito. Contribui tamb\u00e9m para que a argamassa mantenha uma composi\u00e7\u00e3o consistente do in\u00edcio ao fim da aplica\u00e7\u00e3o.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">4. Melhor reten\u00e7\u00e3o do fluxo<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A fluidez inicial \u00e9 importante, mas, por si s\u00f3, n\u00e3o descreve a trabalhabilidade pr\u00e1tica.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os trabalhadores podem precisar de tempo para misturar, transportar, bombear e verter a argamassa. Um material que tenha uma excelente fluidez inicial, mas que perca a maior parte dessa fluidez ap\u00f3s 20 ou 30 minutos, pode provocar um enchimento incompleto.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um \u00e9ter de celulose adequado pode reduzir a perda r\u00e1pida de \u00e1gua e contribuir para um fluxo mais est\u00e1vel ao longo do tempo. Numa f\u00f3rmula devidamente equilibrada, o fluxo aos 30 minutos pode manter-se pr\u00f3ximo do valor inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose, por si s\u00f3, n\u00e3o consegue alcan\u00e7ar este resultado. A composi\u00e7\u00e3o do cimento, a temperatura, o superplastificante, o retardador, a granulometria dos agregados, o teor de \u00e1gua e a energia de mistura tamb\u00e9m afetam a reten\u00e7\u00e3o de fluidez.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">5. Condi\u00e7\u00f5es e hidrata\u00e7\u00e3o mais controladas<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose pode adsorver-se em torno das part\u00edculas de cimento e alterar o movimento da \u00e1gua no sistema. Esta a\u00e7\u00e3o pode influenciar a hidrata\u00e7\u00e3o e a presa do cimento.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Numa dosagem adequada, o efeito pode favorecer uma aplica\u00e7\u00e3o uniforme e reduzir a secagem prematura. Numa dosagem excessiva, o \u00e9ter de celulose pode atrasar a hidrata\u00e7\u00e3o ou reduzir a resist\u00eancia inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Por este motivo, os formuladores devem testar o tempo de presa e a resist\u00eancia ao fim de um dia sempre que alterarem o tipo ou a dosagem do \u00e9ter de celulose.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">De que forma a viscosidade do \u00e9ter de celulose afeta o fluxo da argamassa de inje\u00e7\u00e3o?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A viscosidade \u00e9 um dos fatores de sele\u00e7\u00e3o mais importantes para o \u00e9ter de celulose em argamassas ciment\u00edcias.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um \u00e9ter de celulose de baixa viscosidade provoca uma redu\u00e7\u00e3o menor do fluxo. No entanto, pode n\u00e3o proporcionar um desempenho anti-sangramento suficiente.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um \u00e9ter de celulose de alta viscosidade produz um espessamento mais acentuado com uma dosagem reduzida. No entanto, pode tornar rapidamente uma argamassa autofluida demasiado espessa.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os resultados a seguir ilustram esta rela\u00e7\u00e3o num sistema de argamassa ciment\u00edcia de uso geral.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Viscosidade nominal do \u00e9ter de celulose<\/th><th>Dosagem na mistura seca<\/th><th>Fluxo inicial<\/th><th>Sess\u00e3o de 30 minutos<\/th><th>Observa\u00e7\u00e3o em estado fresco<\/th><\/tr><\/thead><tbody><tr><td>Sem \u00e9ter de celulose<\/td><td>0%<\/td><td>400 mm<\/td><td>N\u00e3o \u00e9 est\u00e1vel<\/td><td>Separa\u00e7\u00e3o vis\u00edvel<\/td><\/tr><tr><td>400<\/td><td>0.03%<\/td><td>370 mm<\/td><td>N\u00e3o \u00e9 est\u00e1vel<\/td><td>Separa\u00e7\u00e3o vis\u00edvel<\/td><\/tr><tr><td>4,000<\/td><td>0.03%<\/td><td>365 mm<\/td><td>370 mm<\/td><td>Fluxo est\u00e1vel<\/td><\/tr><tr><td>40,000<\/td><td>0.03%<\/td><td>330 mm<\/td><td>336 mm<\/td><td>Est\u00e1vel, mas mais espesso<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<figure class=\"wp-block-image aligncenter size-large\"><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"Ensaio de fluidez de argamassa ciment\u00edcia com \u00e9ter de celulose\" class=\"wp-image-2734 lazyload\"\/><noscript><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-1024x576.webp\" alt=\"Ensaio de fluidez de argamassa ciment\u00edcia com \u00e9ter de celulose\" class=\"wp-image-2734\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-1536x865.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Cementitious-Grout-Flow-Test.webp 1890w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose com uma viscosidade nominal de 400 n\u00e3o proporcionou estabiliza\u00e7\u00e3o suficiente numa dosagem de 0,03%. A argamassa continuou a separar-se.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O grau de viscosidade 4 000 proporcionou um equil\u00edbrio mais adequado. Reduziu o caudal inicial de 400 mm para 365 mm, controlando simultaneamente a separa\u00e7\u00e3o. O caudal aos 30 minutos manteve-se pr\u00f3ximo do valor inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O tipo com viscosidade de 40 000 tamb\u00e9m controlou a separa\u00e7\u00e3o, mas reduziu o fluxo de forma mais acentuada. Este tipo pode ser demasiado espesso para uma argamassa que tem de passar por uma abertura estreita.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Estes resultados demonstram por que raz\u00e3o um grau de viscosidade m\u00e9dio-baixa constitui frequentemente um ponto de partida pr\u00e1tico para argamassas ciment\u00edcias de alto fluxo.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">De que forma a dosagem de \u00e9ter de celulose afeta o fluxo da argamassa de rejunte?<\/h2>\n\n\n\n<figure class=\"wp-block-image aligncenter size-large\"><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"Efeito da dosagem de \u00e9ter de celulose no fluxo da argamassa ciment\u00edcia\" class=\"wp-image-2735 lazyload\"\/><noscript><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-1024x576.webp\" alt=\"Efeito da dosagem de \u00e9ter de celulose no fluxo da argamassa ciment\u00edcia\" class=\"wp-image-2735\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-1536x864.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Effect-of-Cellulose-Ether-Dosage-on-Grout-Flow.webp 1891w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A dosagem pode ter um efeito ainda maior do que a viscosidade. O fluxo pode variar lentamente com uma dosagem baixa e, em seguida, diminuir acentuadamente assim que a dosagem ultrapassar um ponto cr\u00edtico.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os dados que se seguem utilizam o mesmo \u00e9ter de celulose com viscosidade nominal de 4 000.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Dosagem do \u00e9ter de celulose<\/th><th>Fluxo inicial<\/th><th>Sess\u00e3o de 30 minutos<\/th><th>Observa\u00e7\u00e3o principal<\/th><\/tr><\/thead><tbody><tr><td>0.01%<\/td><td>380 mm<\/td><td>N\u00e3o \u00e9 est\u00e1vel<\/td><td>Controlo insuficiente da separa\u00e7\u00e3o<\/td><\/tr><tr><td>0.02%<\/td><td>370 mm<\/td><td>375 mm<\/td><td>Esta f\u00f3rmula apresenta um bom equil\u00edbrio<\/td><\/tr><tr><td>0.03%<\/td><td>365 mm<\/td><td>370 mm<\/td><td>Fluxo est\u00e1vel e bom efeito anti-hemorragia<\/td><\/tr><tr><td>0.05%<\/td><td>300 mm<\/td><td>305 mm<\/td><td>Grande redu\u00e7\u00e3o do caudal<\/td><\/tr><tr><td>0.08%<\/td><td>260 mm<\/td><td>262 mm<\/td><td>O caudal \u00e9 demasiado baixo para o objetivo inicial<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">As dosagens de 0,02% e 0,03% produziram os resultados mais equilibrados nesta formula\u00e7\u00e3o espec\u00edfica. A argamassa de inje\u00e7\u00e3o manteve uma elevada fluidez e revelou uma melhor estabilidade.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Quando a dosagem aumentou para 0,05%, o caudal inicial desceu para 300 mm. A 0,08%, desceu para 260 mm. Este n\u00edvel era demasiado baixo para a aplica\u00e7\u00e3o de alto caudal pretendida.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Estas percentagens s\u00e3o pequenas, mas o seu efeito \u00e9 significativo. Numa tonelada m\u00e9trica de argamassa seca:<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Dosagem<\/th><th>\u00c9ter de celulose por tonelada m\u00e9trica<\/th><\/tr><\/thead><tbody><tr><td>0.01%<\/td><td>0,10 kg<\/td><\/tr><tr><td>0.02%<\/td><td>0,20 kg<\/td><\/tr><tr><td>0.03%<\/td><td>0,30 kg<\/td><\/tr><tr><td>0.05%<\/td><td>0,50 kg<\/td><\/tr><tr><td>0.08%<\/td><td>0,80 kg<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">O fabricante deve recorrer a uma pesagem precisa e a uma mistura a seco eficaz. Uma m\u00e1 distribui\u00e7\u00e3o de 200 ou 300 gramas numa tonelada m\u00e9trica pode causar grandes diferen\u00e7as entre os lotes.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O intervalo de 0,02%\u20130,03% pode servir como um intervalo inicial de triagem em laborat\u00f3rio para uma f\u00f3rmula semelhante. N\u00e3o se trata de uma dosagem universal recomendada. Cada produtor deve ajustar a dosagem de acordo com o seu pr\u00f3prio cimento, areia, redutor de \u00e1gua, antiespumante e objetivo de desempenho.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">O \u00e9ter de celulose reduz a resist\u00eancia da argamassa de rejunte?<\/h2>\n\n\n\n<figure class=\"wp-block-image size-large\"><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"Compara\u00e7\u00e3o da exsuda\u00e7\u00e3o de argamassa ciment\u00edcia com \u00e9ter de celulose\" class=\"wp-image-2736 lazyload\"\/><noscript><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-1024x576.webp\" alt=\"Compara\u00e7\u00e3o da exsuda\u00e7\u00e3o de argamassa ciment\u00edcia com \u00e9ter de celulose\" class=\"wp-image-2736\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-1536x865.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Grout-With-and-Without-Cellulose-Ether.webp 1890w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose pode melhorar a reten\u00e7\u00e3o de \u00e1gua e reduzir a segrega\u00e7\u00e3o, mas uma dosagem excessiva pode reduzir a resist\u00eancia mec\u00e2nica.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Existem v\u00e1rios mecanismos que podem causar este resultado:<\/p>\n\n\n\n<ol class=\"wp-block-list\">\n<li>O \u00e9ter de celulose pode introduzir ou estabilizar o ar durante a mistura.<\/li>\n\n\n\n<li>O ar adicional pode aumentar a porosidade da argamassa endurecida.<\/li>\n\n\n\n<li>Uma camada rica em pol\u00edmeros \u00e0 volta das part\u00edculas de cimento pode retardar a hidrata\u00e7\u00e3o inicial.<\/li>\n\n\n\n<li>Uma mistura muito espessa pode n\u00e3o libertar o ar retido de forma eficiente.<\/li>\n\n\n\n<li>Pode ser adicionada \u00e1gua de mistura adicional no local para restabelecer o caudal perdido.<\/li>\n<\/ol>\n\n\n\n<p class=\"wp-block-paragraph\">O efeito final na resist\u00eancia depende, portanto, da dosagem, do teor de ar, do teor de \u00e1gua, da cura e do sistema completo de aditivos.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os resultados que se seguem mostram como a dosagem de um \u00e9ter de celulose com viscosidade nominal de 4 000 afetou a resist\u00eancia inicial.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Dosagem<\/th><th>Resist\u00eancia \u00e0 flex\u00e3o ap\u00f3s 1 dia<\/th><th>Resist\u00eancia \u00e0 compress\u00e3o aos 1 dia<\/th><th>Resist\u00eancia \u00e0 flex\u00e3o aos 3 dias<\/th><th>Resist\u00eancia \u00e0 compress\u00e3o aos 3 dias<\/th><\/tr><\/thead><tbody><tr><td>0%<\/td><td>4,42 MPa<\/td><td>33,50 MPa<\/td><td>4,53 MPa<\/td><td>52,21 MPa<\/td><\/tr><tr><td>0.01%<\/td><td>5,18 MPa<\/td><td>33,26 MPa<\/td><td>5,97 MPa<\/td><td>66,48 MPa<\/td><\/tr><tr><td>0.02%<\/td><td>5,52 MPa<\/td><td>36,61 MPa<\/td><td>7,08 MPa<\/td><td>63,47 MPa<\/td><\/tr><tr><td>0.03%<\/td><td>6,27 MPa<\/td><td>29,56 MPa<\/td><td>7,00 MPa<\/td><td>61,20 MPa<\/td><\/tr><tr><td>0.05%<\/td><td>4,98 MPa<\/td><td>26,68 MPa<\/td><td>6,14 MPa<\/td><td>59,26 MPa<\/td><\/tr><tr><td>0.08%<\/td><td>4,72 MPa<\/td><td>25,98 MPa<\/td><td>4,62 MPa<\/td><td>57,45 MPa<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Uma dosagem baixa e controlada permitiu um desempenho est\u00e1vel neste sistema. Uma dosagem mais elevada provocou uma redu\u00e7\u00e3o evidente na resist\u00eancia \u00e0 compress\u00e3o ao fim de um dia.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Com 0,02%, a resist\u00eancia \u00e0 compress\u00e3o ap\u00f3s um dia atingiu 36,61 MPa. Com 0,08%, baixou para 25,98 MPa. A dosagem elevada tamb\u00e9m reduziu a fluidez, pelo que n\u00e3o proporcionou qualquer vantagem pr\u00e1tica \u00fatil.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um formulador nunca deve avaliar o \u00e9ter de celulose apenas com base na reten\u00e7\u00e3o de \u00e1gua ou na consist\u00eancia visual. O programa de ensaios deve incluir o fluxo inicial, o fluxo retido, a sangria, o teor de ar, o tempo de presa, a expans\u00e3o e a resist\u00eancia inicial e final.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Exemplo de formula\u00e7\u00e3o de argamassa ciment\u00edcia<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">A f\u00f3rmula seguinte pode ser utilizada como refer\u00eancia t\u00e9cnica para um ensaio com argamassa de uso geral.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Mat\u00e9ria-prima<\/th><th>Tipo sugerido<\/th><th>Percentagem<\/th><\/tr><\/thead><tbody><tr><td>Cimento de Portland<\/td><td>Classe de resist\u00eancia 52,5<\/td><td>38.00%<\/td><\/tr><tr><td>Cimento de aluminato de c\u00e1lcio<\/td><td>CA-50<\/td><td>4.00%<\/td><\/tr><tr><td>Gesso anidro<\/td><td>Grau de constru\u00e7\u00e3o<\/td><td>3.00%<\/td><\/tr><tr><td>Agente de resist\u00eancia precoce<\/td><td>Compat\u00edvel com o sistema de cimento<\/td><td>0.05%<\/td><\/tr><tr><td>Areia classificada<\/td><td>Inferior a 2,36 mm<\/td><td>49.17%<\/td><\/tr><tr><td>Superplastificante de policarboxilato<\/td><td>Tipo de p\u00f3<\/td><td>0.30%<\/td><\/tr><tr><td>Antiespumante<\/td><td>Tipo para mistura a seco<\/td><td>0.10%<\/td><\/tr><tr><td>Bentonite modificada<\/td><td>Tipo de material com propriedades reol\u00f3gicas<\/td><td>0.15%<\/td><\/tr><tr><td>Cal viva<\/td><td>Classe de constru\u00e7\u00e3o controlada<\/td><td>5.00%<\/td><\/tr><tr><td>Retardador<\/td><td>Compat\u00edvel com o sistema de aluminatos<\/td><td>0.20%<\/td><\/tr><tr><td>\u00c9ter de celulose<\/td><td><a href=\"https:\/\/zhiweichem.com\/pt\/hpmc\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/hpmc\/\" rel=\"noreferrer noopener\">HPMC<\/a> ou <a href=\"https:\/\/zhiweichem.com\/pt\/hemc\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/hemc\/\" rel=\"noreferrer noopener\">HEMC<\/a><\/td><td>0.03%<\/td><\/tr><tr><td><strong>Mistura seca total<\/strong><\/td><td><\/td><td><strong>100.00%<\/strong><\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Para este tipo de f\u00f3rmula, foi utilizada uma adi\u00e7\u00e3o inicial de \u00e1gua correspondente a cerca de 15% do peso da mistura seca. A necessidade final de \u00e1gua deve ser ajustada em fun\u00e7\u00e3o das mat\u00e9rias-primas e do caudal necess\u00e1rio.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Trata-se de uma refer\u00eancia para o desenvolvimento, n\u00e3o de uma f\u00f3rmula comercial pronta para venda. A reatividade do cimento, a humidade da areia, a pureza do gesso, a atividade da cal e a compatibilidade dos aditivos podem alterar o resultado.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Como se deve realizar um ensaio de fluidez da argamassa de rejunte?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">\u00c9 essencial dispor de um m\u00e9todo de ensaio repet\u00edvel. Pequenas varia\u00e7\u00f5es no tempo de mistura ou na velocidade de ensaio podem dar origem a resultados enganadores.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Um procedimento pr\u00e1tico de laborat\u00f3rio pode seguir os seguintes passos:<\/p>\n\n\n\n<ol class=\"wp-block-list\">\n<li>Aque\u00e7a os materiais secos e a \u00e1gua de mistura at\u00e9 atingirem aproximadamente 20 \u00b0C.<\/li>\n\n\n\n<li>Coloque 1 800 gramas de argamassa seca numa betoneira planet\u00e1ria.<\/li>\n\n\n\n<li>Ligue a batedeira e adicione a \u00e1gua medida no prazo de cerca de 10 segundos.<\/li>\n\n\n\n<li>Misture durante 240 segundos ou siga o procedimento de mistura indicado no produto.<\/li>\n\n\n\n<li>Coloque um cone truncado h\u00famido sobre uma placa de vidro limpa e nivelada.<\/li>\n\n\n\n<li>Encha o cone com argamassa fresca.<\/li>\n\n\n\n<li>Levante o cone na vertical e deixe que a argamassa se espalhe sem vibra\u00e7\u00e3o.<\/li>\n\n\n\n<li>Me\u00e7a o maior di\u00e2metro de expans\u00e3o.<\/li>\n\n\n\n<li>Me\u00e7a um segundo di\u00e2metro perpendicular \u00e0 primeira medi\u00e7\u00e3o.<\/li>\n\n\n\n<li>Utilize a m\u00e9dia dos dois valores como caudal inicial.<\/li>\n\n\n\n<li>Efetue a medi\u00e7\u00e3o inicial no prazo de seis minutos a contar do in\u00edcio da mistura.<\/li>\n\n\n\n<li>Coloque o material de volta na tigela e cubra-o para limitar a evapora\u00e7\u00e3o.<\/li>\n\n\n\n<li>Ap\u00f3s 30 minutos, misture novamente a argamassa durante o per\u00edodo indicado.<\/li>\n\n\n\n<li>Repita a medi\u00e7\u00e3o do espalhamento.<\/li>\n<\/ol>\n\n\n\n<p class=\"wp-block-paragraph\">Em todas as compara\u00e7\u00f5es, devem ser utilizados o mesmo equipamento, a mesma temperatura da \u00e1gua, o mesmo programa de mistura e os mesmos tempos.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Como escolher o tipo adequado de \u00e9ter de celulose da Zhiwei<\/h2>\n\n\n\n<figure class=\"wp-block-image aligncenter size-large\"><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" data-src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-1024x576.webp\" src=\"data:image\/gif;base64,R0lGODlhAQABAIAAAAAAAP\/\/\/yH5BAEAAAAALAAAAAABAAEAAAIBRAA7\" alt=\"HPMC e HEMC da Zhiwei para argamassa ciment\u00edcia\" class=\"wp-image-2739 lazyload\"\/><noscript><img loading=\"lazy\" decoding=\"async\" width=\"1024\" height=\"576\" src=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-1024x576.webp\" alt=\"HPMC e HEMC da Zhiwei para argamassa ciment\u00edcia\" class=\"wp-image-2739\" srcset=\"https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-1024x576.webp 1024w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-300x169.webp 300w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-768x432.webp 768w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-1536x865.webp 1536w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout-18x10.webp 18w, https:\/\/zhiweichem.com\/wp-content\/uploads\/2026\/07\/Zhiwei-Cellulose-Ether-Selection-for-Cementitious-Grout.webp 1890w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/><\/noscript><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">A Zhiwei (Jinan) New Materials Co., Ltd. fornece HPMC e HEMC em diferentes graus de viscosidade. A atual <a href=\"https:\/\/zhiweichem.com\/pt\/hpmc\/\">Gama de HPMC da Zhiwei<\/a> inclui HPMC 400, <a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hpmc-4k\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hpmc-4k\/\" rel=\"noreferrer noopener\">HPMC 4K,<\/a> HPMC 40K, HPMC 100K e outros tipos de alta viscosidade. O <a href=\"https:\/\/zhiweichem.com\/pt\/hemc\/\">Gama Zhiwei HEMC<\/a> inclui o HEMC 400, o HEMC 4K, o HEMC 30K, o HEMC 60K, o HEMC 100H, o HEMC 150H e o HEMC 200H.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Para uma argamassa ciment\u00edcia de elevada fluidez, HPMC 4K ou <a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hemc-4k\/\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hemc-4k\/\" target=\"_blank\" rel=\"noreferrer noopener\">HEMC 4K<\/a> \u00e9 uma primeira op\u00e7\u00e3o l\u00f3gica de sele\u00e7\u00e3o. Estas classes podem proporcionar um maior controlo reol\u00f3gico do que um produto da classe 400, sem a forte redu\u00e7\u00e3o do fluxo associada a uma viscosidade muito elevada <a href=\"https:\/\/en.wikipedia.org\/wiki\/Ethyl_methyl_cellulose\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/en.wikipedia.org\/wiki\/Ethyl_methyl_cellulose\" rel=\"noreferrer noopener\">\u00e9ter de celulose<\/a>.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><thead><tr><th>Objetivo de Desenvolvimento<\/th><th>Orienta\u00e7\u00e3o do N\u00edvel Zhiwei<\/th><th>Considera\u00e7\u00e3o importante<\/th><\/tr><\/thead><tbody><tr><td>Argamassa de alto fluxo com controlo de sangramento<\/td><td>HPMC 4K ou HEMC 4K<\/td><td>Comece com uma dosagem baixa e verifique o fluxo de reten\u00e7\u00e3o<\/td><\/tr><tr><td>Baixa necessidade de espessamento<\/td><td><a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hpmc-400\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hpmc-400\/\" rel=\"noreferrer noopener\">HPMC 400<\/a> ou <a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hemc-400\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hemc-400\/\" rel=\"noreferrer noopener\">HEMC 400<\/a><\/td><td>Pode n\u00e3o conseguir estancar a hemorragia com uma dosagem muito baixa<\/td><\/tr><tr><td>Aumento mais acentuado da viscosidade<\/td><td><a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hpmc-40k\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hpmc-40k\/\" rel=\"noreferrer noopener\">HPMC 40K<\/a> ou <a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hemc-30k\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hemc-30k\/\" rel=\"noreferrer noopener\">HEMC 30K<\/a><\/td><td>Utilize uma dosagem mais baixa e controle cuidadosamente o fluxo<\/td><\/tr><tr><td>Argamassa de alta consist\u00eancia ou argamassa especial n\u00e3o fluida<\/td><td><a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hemc-60k\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hemc-60k\/\" rel=\"noreferrer noopener\">HEMC 60K<\/a> ou superior<\/td><td>Normalmente, n\u00e3o \u00e9 a primeira escolha para argamassa autofluida<\/td><\/tr><tr><td><a href=\"https:\/\/zhiweichem.com\/pt\/hemc\/hemc-para-argamassa-de-reparacao\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/hemc\/hemc-for-repair-mortar\/\" rel=\"noreferrer noopener\">Argamassa para repara\u00e7\u00e3o vertical ou de espessura elevada<\/a><\/td><td>HPMC 100K ou HEMC de alta viscosidade<\/td><td>Mais adequado para objetivos relacionados com o corpo e o combate \u00e0 flacidez<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/zhiweichem.com\/pt\/produtos\/hpmc-100k\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/products\/hpmc-100k\/\" rel=\"noreferrer noopener\">Zhiwei HPMC 100K<\/a> foi concebido para sistemas de constru\u00e7\u00e3o que requerem maior reten\u00e7\u00e3o de \u00e1gua, tempo de trabalho e estabilidade vertical. Estas caracter\u00edsticas s\u00e3o \u00fateis em colas para azulejos, reboco, massa para paredes, argamassa para sistemas de isolamento t\u00e9rmico exterior (EIFS) e argamassa de repara\u00e7\u00e3o. No entanto, um produto de elevada viscosidade como o HPMC 100K pode reduzir excessivamente o fluxo de uma argamassa autonivelante.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O modelo correto deve ser selecionado atrav\u00e9s de ensaios comparativos. O ensaio deve utilizar o cimento, os agregados, o superplastificante, o antiespumante e a propor\u00e7\u00e3o de \u00e1gua reais do cliente, bem como o seu processo de mistura.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">HPMC ou HEMC: qual \u00e9 a melhor op\u00e7\u00e3o para argamassa ciment\u00edcia?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Tanto o HPMC como o HEMC s\u00e3o \u00e9teres de celulose n\u00e3o i\u00f4nicos que podem melhorar a reten\u00e7\u00e3o de \u00e1gua, a viscosidade e a estabilidade em estado fresco nos sistemas de cimento.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Nenhum dos dois tipos \u00e9 automaticamente melhor para todos os tipos de argamassa.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O HPMC \u00e9 amplamente utilizado em <a href=\"https:\/\/zhiweichem.com\/pt\/hpmc\/hpmc-em-materiais-de-construcao\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/hpmc\/hpmc-in-construction-materials\/\" rel=\"noreferrer noopener\">materiais de constru\u00e7\u00e3o de mistura a seco.<\/a> Oferece v\u00e1rias op\u00e7\u00f5es de viscosidade e permite uma reten\u00e7\u00e3o de \u00e1gua fi\u00e1vel, bem como um controlo reol\u00f3gico.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O HEMC tamb\u00e9m pode proporcionar uma reten\u00e7\u00e3o de \u00e1gua e uma trabalhabilidade eficazes. O seu desempenho a temperaturas elevadas pode diferir do de um tipo de HPMC compar\u00e1vel, uma vez que a sua composi\u00e7\u00e3o qu\u00edmica de substitui\u00e7\u00e3o \u00e9 diferente.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A melhor escolha depende de:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Caudal inicial necess\u00e1rio<\/li>\n\n\n\n<li>Fluxo obrigat\u00f3rio de 30 minutos<\/li>\n\n\n\n<li>Temperatura de coloca\u00e7\u00e3o<\/li>\n\n\n\n<li>Teor de cimento e de cimento de aluminato de c\u00e1lcio<\/li>\n\n\n\n<li>Qu\u00edmica dos superplastificantes<\/li>\n\n\n\n<li>Tempo de endurecimento pretendido<\/li>\n\n\n\n<li>Limite de sangramento<\/li>\n\n\n\n<li>Valor-alvo do teor de ar<\/li>\n\n\n\n<li>Requisito de resist\u00eancia inicial<\/li>\n\n\n\n<li>Custo dos materiais<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">Um teste comparativo entre o Zhiwei HPMC 4K e o HEMC 4K pode constituir um ponto de partida \u00fatil para a compara\u00e7\u00e3o.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Como se deve adicionar o \u00e9ter de celulose \u00e0 mistura seca?<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose deve ser distribu\u00eddo uniformemente pelo p\u00f3 seco antes de se adicionar \u00e1gua.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">O produtor pode, em primeiro lugar, pr\u00e9-misturar o \u00e9ter de celulose com cimento, um enchimento fino ou outro p\u00f3 compat\u00edvel. Esta pr\u00e9-mistura pode, em seguida, ser adicionada ao lote principal. Este m\u00e9todo reduz o risco de sobredosagem local.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A equipa de produ\u00e7\u00e3o deve tamb\u00e9m:<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>Utilize uma balan\u00e7a capaz de medir com precis\u00e3o pequenas quantidades<\/li>\n\n\n\n<li>Confirmar a efici\u00eancia de distribui\u00e7\u00e3o do misturador<\/li>\n\n\n\n<li>Evite adicionar \u00e9ter de celulose diretamente numa pequena \u00e1rea do misturador<\/li>\n\n\n\n<li>Mantenha as mat\u00e9rias-primas secas<\/li>\n\n\n\n<li>Controlar o tempo de mistura<\/li>\n\n\n\n<li>Verifique a uniformidade das amostras recolhidas em diferentes partes do lote<\/li>\n\n\n\n<li>Proteger o produto acabado da humidade<\/li>\n<\/ul>\n\n\n\n<p class=\"wp-block-paragraph\">Uma argamassa que cont\u00e9m apenas 0,02% de \u00e9ter de celulose requer um controlo rigoroso da produ\u00e7\u00e3o. Uma distribui\u00e7\u00e3o desigual pode fazer com que um saco fique demasiado l\u00edquido, enquanto outro fica demasiado espesso.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Erros comuns na formula\u00e7\u00e3o<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Escolher o \u00e9ter de celulose apenas com base na viscosidade<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A viscosidade \u00e9 importante, mas n\u00e3o \u00e9 a \u00fanica propriedade. O tamanho das part\u00edculas, o comportamento de dissolu\u00e7\u00e3o, o n\u00edvel de substitui\u00e7\u00e3o, a humidade, a temperatura de gelifica\u00e7\u00e3o e a intera\u00e7\u00e3o com outros aditivos tamb\u00e9m afetam o desempenho.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Dois produtos com a mesma indica\u00e7\u00e3o de viscosidade podem n\u00e3o produzir o mesmo resultado na argamassa de rejunte.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Utiliza\u00e7\u00e3o excessiva de \u00e9ter de celulose<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Uma dosagem mais elevada pode melhorar o desempenho anti-sangramento, mas tamb\u00e9m pode reduzir a fluidez e a resist\u00eancia inicial. A dosagem deve deixar de aumentar assim que a argamassa atingir a estabilidade necess\u00e1ria.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Adicionar mais \u00e1gua para recuperar o caudal<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Os trabalhadores podem adicionar \u00e1gua extra quando a argamassa parecer demasiado espessa. Esta a\u00e7\u00e3o pode aumentar a exsuda\u00e7\u00e3o, o encolhimento e a porosidade. Pode tamb\u00e9m reduzir a resist\u00eancia \u00e0 compress\u00e3o.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A solu\u00e7\u00e3o correta consiste em ajustar o equil\u00edbrio entre o \u00e9ter de celulose e o superplastificante na f\u00f3rmula.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Ignorar a intera\u00e7\u00e3o com o superplastificante<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Os superplastificantes de policarboxilato proporcionam um elevado fluxo com um baixo teor de \u00e1gua. O \u00e9ter de celulose aumenta a viscosidade e pode alterar o modo de funcionamento do superplastificante.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Os dois aditivos devem ser otimizados em conjunto.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Ignorando o teor de ar<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose pode estabilizar o ar introduzido durante a mistura. Pode ser necess\u00e1rio utilizar um antiespumante em p\u00f3 compat\u00edvel para controlar o teor de ar e preservar a resist\u00eancia.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Uma quantidade excessiva de antiespumante tamb\u00e9m pode afetar a qualidade da superf\u00edcie e o fluxo. O fabricante deve testar o sistema na sua totalidade.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Teste apenas do fluxo inicial<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A fluidez inicial n\u00e3o permite determinar se a argamassa de inje\u00e7\u00e3o se manter\u00e1 male\u00e1vel durante a constru\u00e7\u00e3o. O laborat\u00f3rio deve tamb\u00e9m medir a fluidez aos 30 minutos e inspecionar o material para detetar sangramento e segrega\u00e7\u00e3o.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Compara\u00e7\u00e3o de notas em diferentes condi\u00e7\u00f5es de exame<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A temperatura da \u00e1gua, a energia de mistura, o tempo de repouso e o momento da medi\u00e7\u00e3o afetam o resultado. Cada lote deve ser testado nas mesmas condi\u00e7\u00f5es.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Um Processo Pr\u00e1tico de Desenvolvimento de Produtos<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">Um fabricante de argamassa pode utilizar o seguinte processo para selecionar o \u00e9ter de celulose.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 1: Definir as metas de desempenho<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Estabele\u00e7a objetivos claros para o fluxo inicial, o fluxo aos 30 minutos, a sangria, o tempo de presa, a expans\u00e3o, a resist\u00eancia ao fim de um dia, a resist\u00eancia ao fim de tr\u00eas dias e a resist\u00eancia final.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 2: Testar uma f\u00f3rmula sem \u00e9ter de celulose<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A amostra de controlo mostra o fluxo, a sangria e a resist\u00eancia originais. Mostra tamb\u00e9m a corre\u00e7\u00e3o reol\u00f3gica necess\u00e1ria para a f\u00f3rmula.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 3: Selecionar diferentes graus de viscosidade<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Compare um tipo de viscosidade baixa, um de viscosidade m\u00e9dia-baixa e um de viscosidade m\u00e9dia, na mesma dosagem.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Por exemplo, o laborat\u00f3rio pode comparar o Zhiwei HPMC 400, o HPMC 4K e o HPMC 40K.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 4: Otimizar a dosagem<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Ap\u00f3s selecionar o intervalo de viscosidade mais adequado, teste v\u00e1rios n\u00edveis de dosagem. Uma sequ\u00eancia inicial \u00fatil pode incluir 0,01%, 0,02%, 0,03% e 0,05%.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 5: Otimizar o antiespumante e o superplastificante<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Ajuste o superplastificante de forma a atingir a fluidez necess\u00e1ria sem adicionar \u00e1gua desnecess\u00e1ria. Ajuste o antiespumante para controlar o ar sem comprometer a estabilidade.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 6: Confirmar a resist\u00eancia e a durabilidade<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Testar a resist\u00eancia \u00e0 compress\u00e3o inicial e final. O fabricante deve tamb\u00e9m avaliar a expans\u00e3o, a ader\u00eancia, a retra\u00e7\u00e3o e a durabilidade, sempre que a aplica\u00e7\u00e3o exija essas propriedades.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Passo 7: Realizar um teste \u00e0 escala de produ\u00e7\u00e3o<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">A mistura em laborat\u00f3rio e a mistura na f\u00e1brica nem sempre produzem a mesma distribui\u00e7\u00e3o. Um ensaio de produ\u00e7\u00e3o pode confirmar a precis\u00e3o da dosagem, o tempo de mistura, a consist\u00eancia dos sacos e o desempenho no local.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Perguntas mais frequentes<\/h2>\n\n\n\n<h3 class=\"wp-block-heading\">Qual \u00e9 a principal fun\u00e7\u00e3o do \u00e9ter de celulose na argamassa ciment\u00edcia?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">As suas principais fun\u00e7\u00f5es s\u00e3o a reten\u00e7\u00e3o de \u00e1gua, o controlo da viscosidade, o aumento da coes\u00e3o, a redu\u00e7\u00e3o do sangramento e uma melhor reten\u00e7\u00e3o do fluxo.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">O \u00e9ter de celulose reduz sempre a fluidez da argamassa?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose reduz normalmente o caudal em certa medida, uma vez que aumenta a viscosidade da fase aquosa. Essa redu\u00e7\u00e3o pode ser reduzida se a viscosidade e a dosagem forem adequadas. Uma viscosidade ou dosagem excessivas podem provocar uma perda acentuada do caudal.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Qual \u00e9 a dosagem adequada de \u00e9ter de celulose para argamassa ciment\u00edcia?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Uma dosagem de 0,02%\u20130,03% proporcionou um equil\u00edbrio adequado na formula\u00e7\u00e3o de exemplo. Este intervalo deve ser utilizado apenas como ponto de partida laboratorial. A dosagem final depende da f\u00f3rmula completa.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Qual \u00e9 o n\u00edvel do Zhiwei que deve ser avaliado em primeiro lugar?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O Zhiwei HPMC 4K ou HEMC 4K constitui uma op\u00e7\u00e3o pr\u00e1tica para uma primeira avalia\u00e7\u00e3o em betumes ciment\u00edcios de alto fluxo. O cliente deve confirmar a escolha atrav\u00e9s de ensaios de aplica\u00e7\u00e3o.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">O HPMC pode impedir o sangramento da argamassa?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O HPMC pode reduzir significativamente o sangramento quando a sua viscosidade e dosagem s\u00e3o adequadas. Um tipo com viscosidade demasiado baixa pode n\u00e3o proporcionar estabiliza\u00e7\u00e3o suficiente.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Um HPMC de maior viscosidade proporciona um melhor desempenho?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">N\u00e3o necessariamente. Um HPMC de alta viscosidade proporciona um espessamento mais forte, mas pode reduzir a fluidez para um n\u00edvel inferior ao exigido na constru\u00e7\u00e3o. O melhor tipo \u00e9 aquele que cumpre tanto os objetivos de estabilidade como os de fluidez.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">O \u00e9ter de celulose pode melhorar a resist\u00eancia \u00e0 compress\u00e3o?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">Uma dosagem adequada pode contribuir para a hidrata\u00e7\u00e3o e reduzir a segrega\u00e7\u00e3o. No entanto, o \u00e9ter de celulose n\u00e3o garante uma maior resist\u00eancia \u00e0 compress\u00e3o. Uma dosagem excessiva pode aumentar a presen\u00e7a de ar e a porosidade, o que pode reduzir a resist\u00eancia.<\/p>\n\n\n\n<h3 class=\"wp-block-heading\">Por que raz\u00e3o deve ser testado o fluxo de 30 minutos?<\/h3>\n\n\n\n<p class=\"wp-block-paragraph\">O ensaio de fluidez de 30 minutos permite verificar se a argamassa de rejunte se manter\u00e1 male\u00e1vel durante a mistura, o transporte e a aplica\u00e7\u00e3o. Uma fluidez inicial elevada n\u00e3o garante a reten\u00e7\u00e3o pr\u00e1tica dessa fluidez.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">Conclus\u00e3o<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\">O \u00e9ter de celulose \u00e9 um componente pequeno, mas importante, na argamassa ciment\u00edcia. Pode melhorar a reten\u00e7\u00e3o de \u00e1gua, a coes\u00e3o, a resist\u00eancia \u00e0 sangria e a reten\u00e7\u00e3o de fluidez. Estas vantagens ajudam a argamassa a formar uma estrutura endurecida mais uniforme e fi\u00e1vel.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">No entanto, a escolha deve ser precisa. Um produto de baixa viscosidade pode n\u00e3o impedir a separa\u00e7\u00e3o. Um produto de alta viscosidade ou uma dosagem excessiva podem reduzir o fluxo e a resist\u00eancia inicial.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">No caso de argamassas ciment\u00edcias de alto fluxo, um tipo de viscosidade m\u00e9dia-baixa, como o Zhiwei HPMC 4K ou o HEMC 4K, constitui um ponto de partida pr\u00e1tico. O produtor deve, em seguida, otimizar a dosagem em conjunto com o superplastificante de policarboxilato e o antiespumante.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><a href=\"https:\/\/zhiweichem.com\/pt\/sobre-a-zhiwei-jinan\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/about-zhiwei-jinan\/\" rel=\"noreferrer noopener\">Zhiwei (Jinan) New Materials Co., Ltd.<\/a> pode fornecer op\u00e7\u00f5es de HPMC e HEMC para diferentes sistemas \u00e0 base de cimento. Os clientes podem apresentar a sua f\u00f3rmula de base, a fluidez pretendida, o tempo de trabalho, os requisitos de resist\u00eancia e a temperatura de aplica\u00e7\u00e3o. A equipa da Zhiwei poder\u00e1 ent\u00e3o recomendar um <a href=\"https:\/\/zhiweichem.com\/pt\/contacto\/\" target=\"_blank\" data-type=\"link\" data-id=\"https:\/\/zhiweichem.com\/contact\/\" rel=\"noreferrer noopener\">plano de amostragem espec\u00edfico <\/a>para an\u00e1lise laboratorial.<\/p>","protected":false},"excerpt":{"rendered":"<p>Cellulose ether helps cementitious grout retain water, resist bleeding, maintain cohesion, and stay workable during placement. However, cellulose ether does not improve every property at every dosage. A grade with very low viscosity may not provide enough thickening to stop segregation. A grade with very high viscosity can reduce flow so much that the grout [&hellip;]<\/p>\n","protected":false},"author":2,"featured_media":2733,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"footnotes":""},"categories":[119],"tags":[124,120,123,122,121,125],"class_list":["post-2729","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-cementitious-grout","tag-cellulose-ether-dosage","tag-cellulose-ether-in-cementitious-grout","tag-cement-grout-additives","tag-hemc-for-cementitious-grout","tag-hpmc-for-cementitious-grout","tag-non-shrink-grout-formulation"],"acf":[],"_links":{"self":[{"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/posts\/2729","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/comments?post=2729"}],"version-history":[{"count":0,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/posts\/2729\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/media\/2733"}],"wp:attachment":[{"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/media?parent=2729"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/categories?post=2729"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/zhiweichem.com\/pt\/wp-json\/wp\/v2\/tags?post=2729"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}